The physical properties of raw materials are very important for people in our carrier tape industry. Today, we will recommend some real knowledge – list of physical properties of common materials. With these, are you still worried about not forming? List of physical properties of common materials of carrier tape
ABS melt temperature: 210 ℃ – 245 ℃; baking temperature: 90 ℃; baking time: ≥ 2H; mold temperature: 25 ℃ – 75 ℃; molding pressure: medium and high pressure; speed: medium and high speed
ABS flame retardant melt adhesive temperature: 200 ℃ – 230 ℃, baking temperature: 80 ℃, baking time: ≥ 3h, mold temperature: 50 ℃ – 60 ℃, forming pressure: medium pressure speed: medium speed
ABS + glass fiber melt adhesive temperature: 220 ℃ – 250 ℃, baking temperature: 90 ℃, baking time: ≥ 3h, mold temperature: 50 ℃ – 80 ℃, forming pressure: medium and high pressure, speed: medium and high speed
ABS + as melt temperature: 220 ℃ – 240 ℃, baking temperature: 90 ℃, baking time: ≥ 3h, mold temperature: 60 ℃ – 85 ℃, forming pressure: medium and high pressure, speed: medium and high speed
ABS + PC melt temperature: 240 ℃ – 280 ℃, baking temperature: 110 ℃, baking time: ≥ 4h, mold temperature: 50 ℃ – 100 ℃, forming pressure: medium and high pressure, speed: high speed
Type PA6
PA6 melt temperature: 240 ℃ – 270 ℃, baking temperature: 105 ℃, baking time: ≥ 8h, mold temperature: 80 ℃ – 90 ℃, forming pressure: medium and high pressure, speed: high speed
PA6 + glass fiber melt adhesive temperature: 250 ℃ – 280 ℃, baking temperature: 105 ℃, baking time: ≥ 8h, mold temperature: 80 ℃ – 90 ℃, forming pressure: medium and high pressure, speed: high speed
PA12 type PA12 melt temperature: 240 ℃ – 290 ℃, baking temperature: 85 ℃, baking time: ≥ 5h, mold temperature: 30 ℃ – 40 ℃, forming pressure: medium pressure speed: high speed
PA12 + glass fiber melt adhesive temperature: 240 ℃ – 270 ℃, baking temperature: 85 ℃, baking time: ≥ 5h, mold temperature: 80 ℃ – 90 ℃, forming pressure: medium pressure, speed: high speed
PA66 type PA66 melt temperature: 260 ℃ – 290 ℃, baking temperature: 105 ℃, baking time: ≥ 12h, mold temperature: 70 ℃ – 90 ℃, forming pressure: medium pressure speed: high speed
PA66 + glass fiber glue temperature: 260 ℃ – 280 ℃; baking temperature: 105 ℃; baking time: ≥ 12h; mold temperature: 70 ℃ – 90 ℃; molding pressure: medium pressure speed: high speed
PBT type PBT melt adhesive temperature: 240 ℃ – 270 ℃, baking temperature: 140 ℃, baking time: ≥ 4h, mold temperature: 25 ℃ – 50 ℃, molding pressure: medium pressure speed: high speed PBT + glass fiber melt adhesive temperature: 240 ℃ – 265 ℃, baking temperature: 140 ℃, baking time: ≥ 4h, mold temperature: 25 ℃ – 50 ℃, molding pressure: medium pressure speed: high speed
PC class
PC melt temperature: 260 ℃ – 300 ℃, baking temperature: 120 ℃, baking time: ≥ 4h, mold temperature: 70 ℃ – 120 ℃, forming pressure: high pressure speed: high speed, low speed
PC + glass fiber melt temperature: 260 ℃ – 300 ℃; baking temperature: 120 ℃; baking time: ≥ 4H mold temperature: 70 ℃ – 120 ℃ molding pressure: high pressure speed: high speed PC + PBT melt temperature: 235 ℃ – 285 ℃ baking temperature: 130 ℃ baking time: ≥ 4H mold temperature: 35 ℃ – 95 ℃ molding pressure: medium and high pressure speed: high speed
PE-HD
PE-HD melt temperature: 200 ℃ – 230 ℃, mold temperature: 50 ℃ – 95 ℃, forming pressure: low pressure, speed: high speed
PE-LD
PE-LD melt temperature: 180 ℃ – 220 ℃, mold temperature: 20 ℃ – 40 ℃, forming pressure: medium and high pressure, speed: high speed
Pei class
Pei melt temperature: 340 ℃ – 400 ℃, baking temperature: 150 ℃, baking time: ≥ 4h, mold temperature: 100 ℃ – 175 ℃, forming pressure: medium and high pressure, speed: high speed
Pei + glass fiber glue temperature: 340 ℃ – 420 ℃; baking temperature: 150 ℃; baking time: ≥ 4H; mold temperature: 100 ℃ – 175 ℃; molding pressure: medium and high pressure; speed: high speed
Pet class
PET melt temperature: 265 ℃ – 280 ℃, baking temperature: 120 ℃, baking time: ≥ 4h, mold temperature: 80 ℃ – 120 ℃, molding pressure: medium and low pressure speed: high speed pet + glass fiber melt temperature: 275 ℃ – 290 ℃, baking temperature: 120 ℃, baking time: ≥ 4h, mold temperature: 80 ℃ – 120 ℃, molding pressure: medium and low pressure speed: high speed
PMMA
PMMA melt temperature: 230 ℃ – 260 ℃, baking temperature: 90 ℃, baking time: ≥ 4h, mold temperature: 35 ℃ – 85 ℃, molding pressure: medium pressure speed: medium speed
POM class
POM melt temperature: 190 ℃ – 210 ℃, baking temperature: 90 ℃, baking time: ≥ 2h, mold temperature: 80 ℃ – 100 ℃, molding pressure: medium and low pressure, speed: medium and high speed
POM + glass fiber glue temperature: 190 ℃ – 220 ℃; baking temperature: 90 ℃; baking time: ≥ 2H; mold temperature: 80 ℃ – 100 ℃; molding pressure: medium pressure speed: medium high speed
PP class
PP melt temperature: 220 ℃ – 250 ℃, mold temperature: 40 ℃ – 80 ℃, forming pressure: medium and high pressure, speed: medium speed
PP + glass fiber melt adhesive temperature: 230 ℃ – 250 ℃, baking temperature: 80 ℃, baking time: ≥ 3h, mold temperature: 30 ℃ – 60 ℃, molding pressure: medium and high pressure, speed: medium speed
PPE
PPE melt temperature: 240 ℃ – 300 ℃; baking temperature: 100 ℃; baking time: ≥ 4H; mold temperature: 60 ℃ – 100 ℃; molding pressure: medium high pressure; speed: medium low speed
PPO
PPO melt temperature: 240 ℃ – 300 ℃, baking temperature: 110 ℃, baking time: ≥ 4h, mold temperature: 20 ℃ – 60 ℃, molding pressure: medium high pressure speed: medium low speed
PS class
PS melt temperature: 180 ℃ – 260 ℃, baking temperature: 80 ℃, baking time: ≥ 3H mold temperature: 40 ℃ – 50 ℃, molding pressure: low pressure speed: high speed PS + flame retardant melt temperature: 180 ℃ – 240 ℃, baking temperature: 80 ℃, baking time: ≥ 3H mold temperature: 40 ℃ – 50 ℃, molding pressure: low pressure speed: high speed
PVC
PVC melt temperature: 185 ℃ – 205 ℃, mold temperature: 25 ℃ – 50 ℃, forming pressure: medium and high pressure, speed: low speed
As class
As melt temperature: 200 ℃ – 250 ℃, baking temperature: 80 ℃, baking time: ≥ 2h, mold temperature: 40 ℃ – 80 ℃, forming pressure: medium and low pressure, speed: high speed
As + glass fiber glue temperature: 210 ℃ – 240 ℃; baking temperature: 80 ℃; baking time: ≥ 2H; mold temperature: 40 ℃ – 80 ℃; molding pressure: medium and low pressure; speed: high speed
PPS
PPS melt temperature: 270 ℃ – 300 ℃, baking temperature: 130 ℃, baking time: ≥ 4h, mold temperature: 25 ℃ – 85 ℃, forming pressure: medium and high pressure, speed: low speed
PEEK
Peek melt temperature: 350 ℃ – 380 ℃, baking temperature: 150 ℃, baking time: ≥ 3h, mold temperature: 175 ℃ – 205 ℃, molding pressure: medium high pressure speed: medium speed
PPA
PPA melt temperature: 280 ℃ – 325 ℃, baking temperature: 140 ℃, baking time: ≥ 6h, mold temperature: 90 ℃ – 180 ℃, forming pressure: medium and high pressure, speed: medium and high speed
rubber
Rubber melt temperature: 280 ℃ – 325 ℃, baking temperature: 70 ℃, baking time: ≥ 2h, mold temperature: 20 ℃ – 60 ℃, forming pressure: medium and low pressure, speed: medium and low speed